Monday
Jan112010
Stainless Steel without colored oxide
Process Line for ChemPolish™ of 300 Series Stainless Steel without colored oxide
Step |
Process Line |
Concentration & Temperature |
Time |
Heater Equipment |
Process Equipment |
Exhaust Required |
1. |
Alkaline Clean: Spray MicroClean™ CuL (RD-19) |
25% by volume 120-170°F (50-75°C) |
2-4 Min. |
SS or Quartz - OK Teflon - OK Titanium - OK |
SS - OK PVC - OK PP - OK |
Yes |
---|---|---|---|---|---|---|
OR |
||||||
1A. |
Alkaline Clean Soak tank MicroClean CuLX™ (RD-68) |
25% by volume 120-170°F (50-75°C) |
See above |
No |
||
2. |
Cold Rinses, cascaded can usuallly be sent to drain with only pH adjustment, if needed | |||||
3. |
100% 175°-180° F (80-85° C) |
60-90 Seconds |
Teflon or Quartz – OK Titanium - OK |
PVC - No PP - OK |
Yes |
|
OR |
||||||
3A. |
100% 175°-1800° F (80°-850° C) |
60-120 Seconds |
Teflon or Quartz - OK Titanium - OK |
PVC – No |
Yes |
|
4. |
Cold Rinses, Cascaded, (May need to be treated for pH adjustment, and Nickel removal) | |||||
5. |
(Treatment with 50% commercial 42° Be’ Nitric acid may be required if SS is high carbon, and a black smut is generated. This is room temp, ~30 seconds) | |||||
6. |
Further cold rinse, if required. | |||||
7. |
Dry, Turbine blower preferred, if material can handle force. |